Steel normalizing: processes and features

The steel normalizing process consists of heating steel to the austenitic state, holding it at a set temperature and then cooling it in air. Normalizing is closely related to annealing and is often classed as a type of it, but faster cooling in air produces a finer structure. In hypoeutectoid steels containing less than 0.8% carbon, the normalized structure is a mixture of ferrite and fine pearlite.

In hypereutectoid steels (more than 0.8% carbon), the structure after normalizing consists of sorbite – a fine form of pearlite. Heating above the Acm point dissolves the secondary cementite, and faster cooling in air prevents it from re-forming as a continuous network along the grain boundaries. This heat treatment is used to refine the structure and improve machinability. For steel castings, it is often used instead of hardening and tempering to improve their properties. Normalizing is most widely used for low- and medium-carbon and low-alloy steels; for high-carbon and tool steels, it is mainly used to eliminate the cementite network before further heat treatment.

Stages of the steel normalizing process

Normalizing is carried out in several stages. All operations are performed at metallurgical and metalworking plants equipped with heat treatment furnaces of various designs and other specialised equipment.

  1. Heating. Hypoeutectoid steels are heated to 30–50 °C above the Ac3 point. Hypereutectoid steels are heated to 30–50 °C above the Acm point so that the secondary cementite dissolves in the austenite; overheating should be avoided, as it causes austenite grain growth. The exact temperature depends on the carbon content and any alloying elements present. The critical points are determined from the iron–carbon phase diagram and reference data for the specific steel grade, while continuous cooling transformation (CCT) diagrams are used to predict the structure obtained after cooling. For new steel grades, the calculated values are confirmed experimentally. For carbon and low-alloy steels, the heating time in electric furnaces is usually taken as about 1–1.5 minutes per millimetre of section thickness.
  2. Holding. Holding is the time during which the part remains in the furnace at the set temperature. This stage is needed to heat the load completely and uniformly and to complete the phase transformations. The holding time depends on the steel grade, the dimensions of the part and the heating temperature. For small parts of simple shape, holding for about 15 minutes at the set temperature is usually sufficient.
  3. Cooling. Cooling is mainly carried out in still air; forced air cooling is sometimes used. With faster cooling, austenite decomposes at lower temperatures, producing a finer ferrite–cementite structure. As a result, normalized medium- and high-carbon steels have higher strength and hardness than in the annealed condition. The cooling medium, and therefore the cooling rate, has a significant effect on the structure and properties of the steel: the same steel heated to the same temperature but cooled in different ways will have different properties.

What normalizing of carbon and alloy steels achieves

Normalizing castings, forgings, rolled products, semi-finished products and metal parts provides:

  • complete phase recrystallization of the steel;
  • refinement of the coarse-grained structure formed during hot working – rolling, forging and stamping;
  • reduced banding after rolling and more uniform grain size in forgings;
  • higher resistance to brittle fracture, i.e. a lower ductile-to-brittle transition temperature and higher crack propagation energy;
  • elimination of work hardening after cold working and relief of residual stresses;
  • preparation of the structure for subsequent hardening, if required;
  • improved machinability.

Steel castings are normalized to refine the coarse as-cast structure (including the Widmanstätten structure), reduce residual stresses and improve their response to subsequent heat treatment.

Normalizing steels with different carbon contents

The purpose and specifics of normalizing depend on the steel composition:

  • For low-carbon steels, normalizing effectively replaces annealing: it gives slightly higher hardness, better machinability and a cleaner machined surface.
  • For medium-carbon steel castings, normalizing followed by high-temperature tempering can replace hardening and high-temperature tempering. Its advantages are less distortion and lower internal stresses in the parts and therefore a lower risk of cracking, although the mechanical properties are somewhat lower than after hardening.
  • For air-hardening alloy steels, cooling in air already produces martensite or bainite, so normalizing actually acts as hardening and must be followed by tempering.

Equipment and consumables used for normalizing

The required normalizing temperature and cooling conditions are ensured by:

  • Fuel-fired heating chambers with flat-flame burners operating on the principle of direct or indirect heating. Modern designs use recuperative and regenerative burners.
  • Automatic heating control systems. In electric furnaces, power is controlled by thyristor units.
  • Thermal insulation materials.

Conveyor normalizing furnaces with a protective gas atmosphere are used to normalize small parts. The loading and unloading openings are located below the level of the working chamber, and the loading and unloading vestibules are inclined, which helps to keep the protective gas inside the furnace. The conveyor is a mesh belt made of 3 mm nichrome wire. The parts are cooled in the unloading section of the furnace: the cooling tunnel through which the conveyor passes has double walls with cold running water flowing between them. Protective gas fills the entire furnace, including the loading and unloading sections.

The parts are placed on the conveyor in a single layer, which ensures uniform heating and rapid cooling. When leaving the unloading section, the parts must be at a temperature of no more than 50 °C; at higher temperatures, oxide films form on their surface on contact with air. The conveyor speed is up to 20 cm per minute.

Normalizing, like other heat treatment technologies for castings, rolled products, semi-finished products and metal parts, can be an intermediate or a final operation. In most cases, normalizing is an intermediate process. It is used as a final treatment, for example, in the production of rolled sections such as T-sections, I-beams and channels.

The steel normalizing process is therefore an important stage of heat treatment that significantly improves the mechanical properties of metal, prepares it for further processing and ensures the reliability and durability of finished products.

Need normalizing of metal parts?

KARBAZ performs normalizing of metal products to improve the material structure, increase strength and ductility and obtain stable mechanical properties.